Wrought Aluminum 5257

Image Credit: classicparts.sirv.com
Wrought Aluminum 5257 (AA 5257) is an active 5xxx-series aluminum-magnesium alloy intended for wrought products. Its magnesium-based chemistry provides solid-solution strengthening without precipitation heat treatment, while controlled additions of manganese, chromium, and titanium support processing and microstructural control. The alloy is principally suited to sheet, strip, and other wrought forms where corrosion resistance, forming capability, and a high-quality decorative surface are important. It is commonly considered for visible anodized, painted, or polished components rather than applications requiring the highest structural strength available from aluminum alloys.
| Chemical Composition wt.% | ||
|---|---|---|
| Element | Min | Max |
| Magnesium | 1.2 | 2.0 |
| Manganese | 0.05 | 0.20 |
| Silicon | — | 0.15 |
| Iron | — | 0.20 |
| Chromium | 0.10 | 0.25 |
| Copper | — | 0.05 |
| Zinc | — | 0.10 |
| Titanium | 0.03 | 0.10 |
| Other elements, each | — | 0.03 |
| Other elements, total | — | 0.10 |
| Aluminum | Balance | |
Registered AA material confirms 5257 as an active wrought designation and lists a calculated nominal density. The grade-specific chemical limits below are reported by the supplied 5257 supplier datasheet and should be confirmed against the applicable product specification and mill certificate before procurement. Values are mass percent.
Values below are supplier-reported theoretical or typical values for 5257 unless a condition is stated. Mechanical properties vary materially with temper, gauge, product form, and the applicable specification; use certified product data for design.
Use the button to switch between Metric and US Customary units.
| Physical Properties | Metric |
|---|---|
| Density | 2.70 g/cm³2.70 g/cm³ |
| Mechanical Properties | Metric |
| Modulus of Elasticity | 70 GPa |
| Thermal Properties | Metric |
| Melting Range | 620–655 °C |
| Thermal Conductivity | 142–152 W/m·K |
| Coefficient of Thermal Expansion (20–100 °C) | 23.6 × 10⁻⁶ /°C |
| Specific Heat Capacity | 900 J/kg·K |
| Electrical Properties | Metric |
| Electrical Conductivity | 38–42 % IACS |
Test conditions & data notes
- Density: Calculated nominal density for active wrought alloy designation 5257.
- Melting Range: Supplier-reported theoretical value.
- Thermal Conductivity: Supplier-reported theoretical value.
- Coefficient of Thermal Expansion (20–100 °C): supplier-reported theoretical value.
- Specific Heat Capacity: Supplier-reported theoretical value.
- Electrical Conductivity: Supplier-reported theoretical value.
- Modulus of Elasticity: Supplier-reported theoretical value.
Material Conditions & Tempers
As a non-heat-treatable Al-Mg alloy, 5257 is strengthened principally by cold work. O temper provides the greatest forming latitude; H1x tempers provide progressively higher strength with reduced ductility. The following ranges are supplier-reported and are not substitutes for product-standard minimums.
| Condition | Tensile Strength | Yield / Proof Strength | Notes |
|---|---|---|---|
| O | 150–190 MPa | 60–100 MPa | Annealed condition with the highest reported elongation range of 22–28%. Supplier-reported values; product form and thickness are not stated. |
| H12 | 170–210 MPa | 130–170 MPa | Strain-hardened temper with reported elongation of 14–18%. Supplier-reported values; product form and thickness are not stated. |
| H14 | 190–230 MPa | 150–190 MPa | Half-hard strain-hardened temper with reported elongation of 12–16%. Supplier-reported values; product form and thickness are not stated. |
| H16 | 210–250 MPa | 170–210 MPa | Three-quarter-hard strain-hardened temper with reported elongation of 10–14%. Supplier-reported values; product form and thickness are not stated. |
| H18 | 230–270 MPa | 190–230 MPa | Full-hard strain-hardened temper with reported elongation of 8–12%. Supplier-reported values; product form and thickness are not stated. |
Advantages & Limitations
| Advantages | Limitations |
|---|---|
|
|
Processing & Fabrication
| Process | Description |
|---|---|
| Forming | Use O temper where extensive drawing, stretching, or complex stamping is needed. Higher H tempers can be selected when increased as-supplied strength is more important than maximum forming latitude; validate bend radius and forming limits on the actual gauge. |
| Welding | The supplied datasheet describes good weldability using standard aluminum welding methods and identifies 5356 and 4043 as recommended filler options. Qualify filler selection to the joint, service environment, required finish, and governing procedure. |
| Anodizing and finishing | 5257 is positioned for decorative anodizing and consistent appearance. Maintain clean, scratch-free surfaces and control fabrication residues, weld zones, and pre-treatment because these can alter the finished visual result. |
| Machining | Use sharp tools, stable workholding, and appropriate lubrication to protect the intended cosmetic surface. Chip control and finish should be qualified for the actual temper and product form. |
Applications
AA 5257 is appropriate where a wrought Al-Mg alloy must combine corrosion resistance and fabrication capability with an appearance-sensitive finished surface. Selection should be confirmed against the required form, temper, mechanical-property minimums, finishing route, and environmental exposure.
- Automotive decorative trim: Formability and the reported suitability for consistent anodized or polished appearance support visible moldings, surrounds, and interior trim.
- Architectural trim and decorative panels: The alloy’s corrosion resistance and finishing response are useful for non-primary-structural interior or exterior appearance components.
- Appliance and consumer-product bezels: Wrought sheet can be formed into light cosmetic housings, handles, and trim where surface quality is important.
- Nameplates, signage, and display components: Decorative anodizing capability and sheet-forming versatility suit thin, visible fabricated parts.
Standards & Designations
| Designation | Value | Description |
|---|---|---|
| Aluminum Association | AA 5257 | Active wrought aluminum alloy designation listed in the Aluminum Association Teal Sheets (December 2025). |
| European designation | EN AW-5257 | Listed by the supplied supplier datasheet; confirm applicability in the current governing EN product standard. |
| Japanese designation | JIS A5257 | Listed by the supplied supplier datasheet; verify against the applicable current JIS standard before specification. |
| ISO | ISO 6361-2 | Referenced by the supplied supplier datasheet; confirm product scope and alloy inclusion in the current edition. |
Frequently Asked Questions
Is wrought aluminum 5257 heat treatable?
No. 5257 is a 5xxx Al-Mg alloy and is not strengthened by precipitation heat treatment. Its strength is adjusted primarily by strain hardening, expressed through tempers such as H12, H14, H16, and H18.
Which 5257 temper is best for deep forming?
O temper is generally the practical starting point for demanding drawing and complex stamping because it has the greatest reported elongation. Final selection must account for sheet gauge, part geometry, bend radius, tooling, and the required post-forming strength.
Why is 5257 considered for decorative parts?
The supplied 5257 datasheet specifically identifies high surface quality, polishing behavior, and decorative anodizing response. These traits make it relevant to visible trim, panels, bezels, and signage, provided surface handling and finishing controls are maintained.
References & Data Notes
- (n.d.). The Aluminum Association — International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys, Teal Sheets, December 2025. https://www.aluminum.org/sites/default/files/2026-01/Teal%20Sheets%20December%202025.pdf
- (n.d.). 5257 Aluminum alloy technical datasheet. https://hjelements.com/aluminium-metal-and-alloys/5257-aluminum-alloy,aluminum-5257-alloy,ai-alloy.html
Chemical limits and several physical/mechanical values are drawn from the supplied 5257 supplier datasheet. The Aluminum Association Teal Sheets source supports 5257 as an active wrought designation and its calculated nominal density. Confirm chemistry, temper, dimensions, mechanical minimums, finish, and applicable standard on the supplier’s mill test certificate and purchase specification.